62Sn36Pb2Ag versus Sn63Pb37 We didn’t have the same composition for you. Please just refer below data Basic Properties ü Cross-section view (SEM) Sn/37Pb Sn/37Pb/2Ag Melting Temp. (℃) 183 179~180 Density (g/cm3) 8.40 8.44 Vicker’s Hardness (Hv) 12 13.1 Elongation (%) 45 31 Tensile Strength (Mpa) 40 47.6 Thermal Exp. (x10-6/k) 21 25.7 Electrical Resistivity (μohm·cm) 14.5 14.8 Sn37Pb Pb-rich AuSn4 Sn37Pb2Ag § Sn37Pb2Ag have higher hardness and tensile strength than Sn37Pb because of Ag3Sn precipitates in solder bulk. § Therefore, Sn37Pb2Ag solder has higher mechanical strength and thermal cycle performance. RealValueä MK Electron Co, Ltd. 2011 Beyond the Perfection TM u Test condition & Result - Thermal cycling test : 155/-45℃, 15/15min - Ball size : 640um § Sn37Pb2Ag showed higher shear strength and low reduction rate of strength than Sn37Pb during thermal cycling. § As a result, Ag have benefit for mechanical strength and thermal cycling performance RealValueä MK Electron Co, Ltd. 2011 Beyond the Perfection TM